ASTM B345/B345M-11 - 1.8.2011
 
1. Scope

1.1 This specification covers seamless pipe and seamless extruded tube in the aluminum and aluminum alloys (Note 1) and tempers listed in Table 1 and Table 2, respectively. Seamless pipe and seamless tube are intended for use in applications involving internal pressure.

Note 1—Throughout this specification use of the term alloy in the general sense includes aluminum as well as aluminum alloy.

Note 2—For drawn seamless tubes, see Specifications B210 and B210M; for extruded tubes, Specifications B221 and B221M; for drawn seamless tubes for condensers and heat exchangers, Specifications B234 and B234M; for seamless pipe and seamless extruded tube, B241/B241M; for round welded tubes, Specification B313/B313M; for seamless condenser and heat exchanger tubes with integral fins, Specification ; for extruded structural pipe and tube, Specification B429/B429M; and for drawn tube for general purpose applications, Specification B483/B483M.

1.2 Alloy and temper designations are in accordance with ANSI H35.1 [H35.1M]. The equivalent Unified Numbering System alloy designations are those of Table 3 preceded by A9, for example, A93003 for aluminum alloy 3003 in accordance with Practice E527.

1.3 For acceptance criteria for inclusion of new aluminum and aluminum alloys in this specification, see Annex A2.

1.4 The values stated in either inch-pound units or SI units are to be regarded separately as standard. Within the text, the SI units are shown in brackets. The values stated in each system are not exact equivalents; therefore, each system shall be used independently of the other. Combining values from the two systems may result in nonconformance with the specification.

TABLE 1 Tensile Property Limits for Extruded Seamless PipeA,B

AlloyTemperPipe Size,
in.
Strength, min, ksi [MPa]ElongationC,D
TensileYield (0.2 % Offset)in 2 in. [50 mm] or 4×
Diameter, min, %
in 5 × D
(5.65 )

3003

H18

under 1

27.0 [185]

24.0 [165]

4

4

H112

1 and over

14.0 [95]

5.0 [35]

25

22

6061

T6

under 1

38.0 [260]

35.0 [240]

8

...

1 and over

38.0 [260]

35.0 [240]

10E

9

6063

T6

all

30.0 [205]

25.0 [170]

8

7

6351

T5
T6

all
all

38.0 [260]
42.0 [290]

35.0 [240]
37.0 [255]

10E
10F

9
9

A The basis for establishment of mechanical property limits is given in Annex A1 of this specification.

B To determine conformance to this specification, each value for tensile strength and for yield strength shall be rounded to the nearest 0.1 ksi [MPa] and each value for elongation to the nearest 0.5 %, both in accordance with the rounding method of Practice E29.

C Elongation of full-section and sheet-type specimens is measured in 2 in.; of cut-out round specimens, 4× specimen diameter.

D Elongations in 50 mm apply for pipe tested in full sections and for sheet-type specimens machined from material up through 12.5 mm in thickness having parallel surfaces. Elongations in 5 × D (at 5.65 ), where D and A are diameter and cross-sectional area of the specimen, respectively, apply to round test specimens machined from thicknesses over 6.30 mm.

E The minimum elongation for a wall thickness up through 0.249 in. [6.3 mm] is 8 %.

F For wall thickness 0.124 in. [3.20 mm] and less, the minimum elongation is 8 %.

TABLE 2 Tensile Property Limits for Extruded Seamless TubeA,B

Temper Specified Wall
Thickness, in. [mm]
Area, in.2 [mm2]Tensile Strength, ksi [MPa]Yield Strength
(0.2 % offset)
ksi [MPa], min
ElongationC,D
minmaxin 2 in. [50 mm] or
4 × D min,%
in 5 × D
(5.65 )E

Aluminum 1060F

O
H112

all
all

all
all

8.5 [60]
8.5 [60]

14.0 [95]
... [...]

2.5 [15]
2.5 [15]

25
25G

22
22G

Alloy 3003F

O
H112

all
all

all
all

14.0 [95]
14.0 [95]

19.0 [130]
... [...]

5.0 [35]
5.0 [35]

25
25

22
22

Alloy Alclad 3003F

O
H112

all
all

all
all

13.0 [90]
13.0 [90]

18.0 [125]
... [...]

4.5 [30]
4.5 [30]

25
25

22
22

Alloy 5083F

O
H111
H112

all [130.00]
all [130.00]
all [130.00]

up through 32.0 [20 000]
up through 32.0 [20 000]
up through 32.0 [20 000]

39.0 [270]
40.0 [275]
39.0 [270]

51.0 [350]
... [...]
... [...]

16.0 [110]
24.0 [165]
16.0 [110]

14
12
12

12
10
10

Alloy 5086F

O
H111
H112

all [130.00]
all [130.00]
all [130.00]

up through 32.0 [20 000]
up through 32.0 [20 000]
up through 32.0 [20 000]

35.0 [240]
36.0 [250]
35.0 [240]

46.0 [315]
... [...]
... [...]

14.0 [95]
21.0 [145]
14.0 [95]

14
12
12

12
10
10

Alloy 6061F

OH

all

all

... [...]

22.0 [150]

16.0I [...]

16

14

T1

[16.00]

all

[180]

... [...]

[95]

16

14





all


all


26.0 [180]


... [...]


16.0 [110]


16


14

T42J

all

all

26.0 [180]

... [...]

12.0 [85]

16

14

T51

[16.00]

all

[240]

... [...]

[205]

8

7



up through 0.249 [6.30]
0.250 and over [6.30]

all
all

38.0 [260]
38.0 [260]

... [...]
... [...]

35.0 [240]
35.0 [240]

8
10

...
9

Alloy 6063F

OH
T1K

all
up through 0.500 [12.50]
0.501–1.000 [12.50–25.00]

... [all]
all
all

... [...]
17.0 [115]
16.0 [110]

19.0 [130]
... [...]
... [...]

... [...]
9.0 [60]
8.0 [55]

18
12
12 [...]

16
10
10

T4, T42L

up through 0.500 [12.50]

all

19.0 [130]

... [...]

10.0 [70]

14

12

0.501–1.000 [12.50–25.00]

all

18.0 [125]

... [...]

9.0 [60]

14 [...]

12

T5

up through 0.500 [12.50]

all

22.0 [150]

... [...]

16.0 [110]

8

7

0.501–1.000 [12.50–25.0]

all

21.0 [145]

... [...]

15.0 [105]

8 [...]

7

T52

up through 1.000 [25.00]

all

22.0 [150]

30.0 [205]

16.0M [110]

8

7

T6, T62L

up through 0.124 [3.20]

all

30.0 [205]

... [...]

25.0 [170]

8

...

0.125–1.000 [3.20–25.00]

all

30.0 [205]

... [...]

25.0 [170]

10

7

Alloy 6070F

T6, T62L

up through 2.999

up through 32

48.0 [330]

... [...]

45.0 [310]

6

5

Alloy 6351F

T4
T6

all
up through 0.124
0.125–0.749

all
...
...

32.0 [220]
42.0 [290]
42.0 [290]

... [...]
... [...]
... [...]

19.0 [130]
37.0 [255]
37.0 [255]

16
8
10

14
...
9

A The basis of establishment of mechanical property limits is given in Annex A1 of this specification.

B To determine conformance to this specification, each value for ultimate tensile strength and for yield strength shall be rounded to the nearest 0.1 ksi [MPa] and each value for elongation to the nearest 0.5 %, both in accordance with the rounding method of Practice E29.

C Elongation of full-section and sheet-type specimens is measured in 2 in.; of cut-out round specimens, in 4× specimen diameter.

D For material of such dimensions that a standard test specimen cannot be taken, or for material thinner than 0.062 in., the test for elongation is not required.

E Elongations in 50 mm apply for tube tested in full section and for sheet-type specimens machined from material up through 12.5 mm in thickness having parallel surfaces. Elongations in 5× diameter (5.65 ), where D and A are diameter and cross-sectional area of the specimen, respectively, apply to round test specimens machined from thickness over 6.30 mm. For tube of such dimensions that a standard test specimen cannot be taken, the test for elongation is not required.

F These alloys are also produced in the F temper, for which no mechanical properties are specified.

G Maximum tensile strength and minimum elongation apply to tubes having diameters from 1.000 in. to 4.500 in. and wall thickness from 0.050 in. to 0.169 in. only. Minimum elongation applies to tubes having diameters from 25.00 to 115.00 mm and wall thickness over 1.30 through 4.30 mm only.

H Upon heat treatment, annealed (0 temper) material shall be capable of developing the mechanical properties applicable to T42 temper material, and upon solution and precipitation heat treatment shall be capable of developing the mechanical properties applicable to T62 temper material.

I Yield strength is maximum [110 MPa] max.

J For stress-relieved tempers (T4510, T4511, T6510 and T6511) characteristics and properties other than those specified may differ somewhat from the corresponding characteristics and properties of material in the basic temper.

K Formerly designated T42 temper. Properly aged precipitation heat-treated 6063-T1 extruded products are designated T5.

L While material in the T42 and T62 tempers is not available from the material producer, the properties are listed to indicate those which can usually be obtained by the user when the material is properly solution heat treated or solution and precipitation heat treated from the O (annealed) or F (as-fabricated) tempers. These properties apply when samples of material supplied in the O or F temper are heat treated by the producer to the T42 or T62 tempers to determine that the material will respond to proper thermal treatment. Properties attained by the user, however, may be lower than those listed if the material has been formed or otherwise cold or hot worked, particularly in the annealed temper, prior to solution heat treatment.

M Maximum yield strength is 25.0 ksi [170 MPa].

TABLE 3 Chemical CompositionA,B,C

AlloyComposition, %
SiliconIronCopperManganeseMagnesium ChromiumZincVanadiumTitaniumOther ElementsDAluminum
EachTotalE

1060
3003

0.25
0.6

0.35
0.7

0.05
0.05–0.20

0.03
1.0–1.5

0.03
...

...
...

0.05
0.10

0.05
...

0.03
...

0.03
0.05

...
0.15

99.60 minF
remainder

Alclad 3003

3003 alloy clad inside or outside with 7072 alloy

5083

0.40

0.40

0.10

0.40–1.0

4.0–4.9

0.05–0.25

0.25

...

0.15

0.05

0.15

remainder

5086

0.40

0.50

0.10

0.20–0.7

3.5–4.5

0.05–0.25

0.25

...

0.15

0.05

0.15

remainder

6061G

0.40–0.8

0.7

0.15–0.40

0.15

0.8–1.2

0.04–0.35

0.25

...

0.15

0.05

0.15

remainder

6063

0.20–0.6

0.35

0.10

0.10

0.45–0.9

0.10

0.10

...

0.10

0.05

0.15

remainder

6070

1.0–1.7

0.50

0.15–0.40

0.40–1.0

0.50–1.2

0.10

0.25

...

0.15

0.05

0.15

remainder

6351

0.7–1.3

0.50

0.10

0.40–0.8

0.40–0.8

...

0.20

...

0.20

0.05

0.15

remainder

7072H

0.7 Si + Fe

0.10

0.10

0.10

...

0.8–1.3

...

...

0.05

0.15

remainder

A Limits are in percent maximum unless shown as a range or stated otherwise.

B Analysis shall be made for the elements for which limits are shown in this table.

C For purposes of determining conformance to these limits, an observed value or a calculated value obtained from analysis shall be rounded to the nearest unit in the last right-hand place of figures used in expressing the specified limit, in accordance with the rounding method of Practice E29.

D Others includes listed elements for which no specific limit is shown as well as unlisted metallic elements. The producer may analyze samples for trace elements not specified in the specification. However, such analysis is not required and may not cover all metallic Others elements. Should any analysis by the producer or the purchaser establish that an Others element exceeds the limit of Each or that the aggregate of several Others elements exceeds the limit of Total, the material shall be considered non-conforming.

E Other ElementsTotal shall be the sum of unspecified metallic elements 0.010 % or more, rounded to the second decimal before determining the sum.

F The aluminum content shall be calculated by subtracting from 100.00 % the sum of all metallic elements present in amounts of 0.010 % or more each, rounded to the second decimal before determining the sum.

G In 1965 the requirements for Alloy 6062 were combined with those of Alloy 6061 by revision of the minimum chromium content from 0.15 to 0.04. For this reason, Alloy 6062 was cancelled.

H Composition of cladding alloy as applied during the course of manufacture. The sample from finished tube shall not be required to conform to these limits.

 
2. Referenced Documents

E55-23

Standard Practice for Sampling Wrought Nonferrous Metals and Alloys for Determination of Chemical Composition

Fed. Std. No. 123

Marking for Shipment (Civil Agencies)

H35.2M

Dimensional Tolerances for Aluminum Mill Products

MIL-STD-129

Marking for Shipment and Storage Available from Standardization Documents Order Desk, Bldg. 4 Section D, 700 Robbins Ave., Philadelphia, PA 19111-5094, Attn: NPODS.

D 10.7

Recommended Practices for Gas Shielded Arc Welding of Aluminum and Aluminum-Alloy Pipe Available from the American Welding Society, 2501 Northwest 7th St., Miami, FL 33125.

E1251-25

Standard Test Method for Analysis of Aluminum and Aluminum Alloys by Spark Atomic Emission Spectrometry

B483/B483M-21

Standard Specification for Aluminum and Aluminum-Alloy Drawn Tube and Drawn Pipe for General Purpose Applications

B429/B429M-20

Standard Specification for Aluminum-Alloy Extruded Structural Pipe and Tube

E18-25

Standard Test Methods for Rockwell Hardness of Metallic Materials

B313-B313M-09

Standard Specification for Aluminum and Aluminum-Alloy Round Welded Tubes (Withdrawn 2018)

B404-B404M-02

Standard Specification for Aluminum and Aluminum-Alloy Seamless Condenser and Heat-Exchanger Tubes with Integral Fins (Withdrawn 2006)

B210M-12

Standard Specification for Aluminum and Aluminum-Alloy Drawn Seamless Tubes (Metric) (Withdrawn 2019)

B221-21

Standard Specification for Aluminum and Aluminum-Alloy Extruded Bars, Rods, Wire, Profiles, and Tubes

B221M-21

Standard Specification for Aluminum and Aluminum-Alloy Extruded Bars, Rods, Wire, Profiles, and Tubes (Metric)

B210-12

Standard Specification for Aluminum and Aluminum-Alloy Drawn Seamless Tubes

B234-17(2025)

Standard Specification for Aluminum and Aluminum-Alloy Drawn Seamless Tubes for Surface Condensers, Evaporators, and Heat Exchangers

B234M-17(2025)

Standard Specification for Aluminum and Aluminum-Alloy Drawn Seamless Tubes for Surface Condensers, Evaporators, and Heat Exchangers (Metric)

B241/B241M-22

Standard Specification for Aluminum and Aluminum-Alloy Seamless Pipe and Seamless Extruded Tube

E29-22

Standard Practice for Using Significant Digits in Test Data to Determine Conformance with Specifications

E34-11

Standard Test Methods for Chemical Analysis of Aluminum and Aluminum-Base Alloys

E227-90(1996)

Standard Test Method for Optical Emission Spectrometric Analysis of Aluminum and Aluminum Alloys by the Point-to-Plane Technique (Withdrawn 2002)

E527-23

Standard Practice for Numbering Metals and Alloys in the Unified Numbering System (UNS)

E607-02

Standard Test Method for Atomic Emission Spectrometric Analysis Aluminum Alloys by the Point to Plane Technique Nitrogen Atmosphere

B557-15(2023)

Standard Test Methods for Tension Testing Wrought and Cast Aluminum- and Magnesium-Alloy Products

B557M-15(2023)

Standard Test Methods for Tension Testing Wrought and Cast Aluminum- and Magnesium-Alloy Products (Metric)

B647-23

Standard Test Method for Indentation Hardness of Aluminum Alloys by Means of a Webster Hardness Gage

B648-23

Standard Test Method for Indentation Hardness of Aluminum Alloys by Means of a Barcol Impressor

B660-23

Standard Practices for Packaging/Packing of Aluminum and Magnesium Products

B666/B666M-20

Standard Practice for Identification Marking of Aluminum and Magnesium Products

E716-16(2021)e2

Standard Practices for Sampling and Sample Preparation of Aluminum and Aluminum Alloys for Determination of Chemical Composition by Spark Atomic Emission Spectrometry (Includes all amendments and changes 9/7/2022).

B807/B807M-20

Standard Practice for Extrusion Press Solution Heat Treatment for Aluminum Alloys

B918-01

Standard Practice for Heat Treatment of Wrought Aluminum Alloys