1.1 This specification covers plate, sheet, and strip of low-carbon nickel-chromium-molybdenum alloys (UNS N10276, N06022, N06455, N06035, N06044, UNS N06058, UNS N06059), low-carbon nickel-chromium-molybdenum-copper alloy (UNS N06200), low-carbon nickel-molybdenum-chromium (UNS N10362), low-carbon nickel-chromium-molybdenum-tantalum alloy (UNS N06210), and low-carbon nickel-chromium-molybdenum-tungsten alloy (UNS N06686) as shown in Table 1, for use in general corrosive service. TABLE 1 Chemical Requirements Element | Composition Limits, % | Alloy N06035 | Alloy N06044 | Alloy N10276 | Alloy N06022 | Alloy N06455 | Alloy N06059 | Alloy N06058 | Alloy N06200 | Alloy N06210 | Alloy N10362 | Alloy N06686 | Molybdenum | 7.60–9.00 | 0.80-1.20 | 15.0–17.0 | 12.5–14.5 | 14.0–17.0 | 15.0–16.5 | 18.5–21.0 | 15.0–17.0 | 18.0–20.0 | 21.5–23.0 | 15.0-17.0 | Chromium | 32.25–34.25 | 43.5-45.3 | 14.5–16.5 | 20.0–22.5 | 14.0–18.0 | 22.0–24.0 | 20.0–23.0 | 22.0–24.0 | 18.0–20.0 | 13.8–15.6 | 19.0-23.0 | Iron | 2.00 max | 0.3 max | 4.0–7.0 | 2.0–6.0 | 3.0 max | 1.5, max | 1.5, max | 3.0 max | 1.0 max | 1.25 max | 5.0 max | Tungsten | 0.60 max | ... | 3.0–4.5 | 2.5–3.5 | ... | ... | 0.3 max | ... | ... | ... | 3.0-4.4 | Cobalt, max | 1.00 | ... | 2.5 | 2.5 | 2.0 | 0.3 | 0.3 | 2.0 max | 1.0 | ... | ... | Carbon, max | 0.050 | 0.02 | 0.010 | 0.015 | 0.015 | 0.010 | 0.010 | 0.010 | 0.015 | 0.010 | 0.010 | Silicon, max | 0.60 | 0.20 | 0.08 | 0.08 | 0.08 | 0.10 | 0.10 | 0.08 | 0.08 | 0.08 | 0.08 | Manganese, max | 0.50 | 0.07-0.30 | 1.0 | 0.50 | 1.0 | 0.5 | 0.5 | 0.50 | 0.5 | 0.60 | 0.75 | Vanadium, max | 0.20 | ... | 0.35 | 0.35 | ... | ... | ... | ... | 0.35 | ... | ... | Phosphorus, max | 0.030 | 0.020 | 0.04 | 0.02 | 0.04 | 0.015 | 0.015 | 0.025 | 0.02 | 0.025 | 0.04 | Sulfur, max | 0.015 | 0.020 | 0.03 | 0.02 | 0.03 | 0.010 | 0.010 | 0.010 | 0.02 | 0.010 | 0.02 | Titanium | ... | 0.10-0.30 | ... | ... | 0.7 max | ... | ... | ... | ... | ... | 0.02-0.25 | Nickel | remainderA | Bal | remainderA | remainderA | remainderA | Bal | Bal | remainderA | remainderA | remainderA | remainderA | Aluminum | 0.40 max | 0.30 max | ... | ... | ... | 0.1–0.4 | 0.40 max | 0.50 max | ... | 0.50 max | ... | Copper | 0.30 max | ... | ... | ... | ... | 0.50 max | 0.50 max | 1.3–1.9 | ... | ... | ... | Tantalum | ... | ... | ... | ... | ... | ... | ... | ... | 1.5–2.2 | ... | ... | Nitrogen | ... | ... | ... | ... | ... | ... | 0.02–0.15 | | | | | TABLE 2 Mechanical Property Requirements Alloy | Tensile Strength, min, psi (MPa) | Yield Strength (0.2 % Offset), min, psi (MPa) | Elongation in 2 in. (50.8 mm) or 4DA min, % | Rockwell Hardness,B max | N10276 | 100 000 (690) | 41 000 (283) | 40 | 100 HRB | N06022 | 100 000 (690) | 45 000 (310) | 45 | 100 HRB | N06455 | 100 000 (690) | 40 000 (276) | 40 | 100 HRB | N06035 | 85 000 (586) | 35 000 (241) | 30 | 100 HRB | N06044 | 100 000 (690) | 45 000 (310) | 30 | 100 HRB | N06058 | 110 000 (760) | 52 000 (360) | 40 | 100 HRB | N06059 | 100 000 (690) | 45 000 (310) | 45 | 100 HRB | N06200 | 100 000 (690) | 45 000 (310) | 45 | 100 HRB | N10362 | 105 000 (725) | 45 000 (310) | 40 | 100 HRB | N06686 | 100 000 (690) | 45 000 (310) | 45 | 100 HRB | N06210 | 100 000 (690) | 45 000 (310) | 45 | 100 HRB | 1.2 The following products are covered under this specification: 1.2.1 Sheet and Strip—Hot or cold rolled, solution annealed, and descaled unless solution anneal is performed in an atmosphere yielding a bright finish. 1.2.2 Plate—Hot or cold rolled, solution annealed, and descaled. 1.3 The values stated in inch-pound units are to be regarded as standard. The values given in parentheses are mathematical conversions to SI units that are provided for information only and are not considered standard. 1.4 This standard does not purport to address all of the safety concerns, if any, associated with its use. It is the responsibility of the user of this standard to become familiar with all hazards including those identified in the appropriate Safety Data Sheet (SDS) for this product/material as provided by the manufacturer, to establish appropriate safety and health practices, and determine the applicability of regulatory limitations prior to use. 1.5 This international standard was developed in accordance with internationally recognized principles on standardization established in the Decision on Principles for the Development of International Standards, Guides and Recommendations issued by the World Trade Organization Technical Barriers to Trade (TBT) Committee. |
B906-22 | Standard Specification for General Requirements for Flat-Rolled Nickel and Nickel Alloys Plate, Sheet, and Strip |
E140-12B(2019)e1 | Standard Hardness Conversion Tables for Metals Relationship Among Brinell Hardness, Vickers Hardness, Rockwell Hardness, Superficial Hardness, Knoop Hardness, Scleroscope Hardness, and Leeb Hardness (Includes all amendments and changes 5/7/2019). |
E527-23 | Standard Practice for Numbering Metals and Alloys in the Unified Numbering System (UNS) |
E112-25e1 | Standard Test Methods for Determining Average Grain Size (Includes all amendments and changes 9/9/2026). |
|